LOCTITE EA E-20HP

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LOCTITE EA E-20HP

Main features

  • Glass-to-Wood Epoxy Bonding
  • 20-Minute Working Window
  • 20 kV/mm Dielectric Strength

Product Description

LOCTITE® EA E-20HP is a toughened, two-component industrial epoxy adhesive formulated for room-temperature bonding with a practical 20-minute working life at 23°C. The medium-viscosity resin and hardener mix at 2:1 by volume or 100:55 by weight and cure to an off-white bondline. The cured adhesive combines peel resistance, substrate-specific shear strength, chemical and solvent resistance, and electrical insulation. It is intended for general industrial bonding where moderate assembly time is needed across prepared metals, plastics, wood, glass, epoxyglass, dry concrete, and architectural materials. Bond performance depends on substrate condition, surface preparation, bondline, cure, and service environment.

Key features

  • Toughened epoxy system: Forms a tough, off-white bondline with high peel resistance and high shear strength under the specified test conditions.
  • Moderate processing window: Provides a typical working life of 20 minutes at 23°C and a 40-minute tack-free time.
  • Controlled two-part mixing: Mix ratio is 2:1 by volume or 100:55 by weight, resin to hardener.
  • Broad tested substrate set: Typical shear data are available for prepared metals, plastics, wood, epoxyglass, glass, and dry concrete.
  • Electrical insulation: Typical dielectric breakdown strength is 20 kV/mm after the stated cure.
  • Environmental resistance data: Retained lap-shear results are available after exposure to oils, fuel, water/glycol, humidity, water, acetone, and isopropanol.

Applications / Suitable for

General industrial bonding of prepared metals and plastics, dry concrete bonding, wood and glass bonding, epoxyglass assemblies, and architectural-material applications requiring a moderate room-temperature work life.

Technical Specifications

No specifications available.

Additional Information

Industrial epoxy adhesive

LOCTITE® EA E-20HP

A toughened, medium-viscosity, two-component epoxy for general industrial bonding. The 2:1 volume-mix system provides a 20-minute working life at 23°C, cures at room temperature, and develops an off-white bondline with peel resistance, substrate-specific shear strength, electrical insulation, and environmental resistance.

Two-component epoxy 2:1 mix ratio by volume 20 min working life at 23°C Room-temperature cure Medium viscosity Off-white cured bondline

LOCTITE® EA E-20HP two-component epoxy adhesive.

Unmixed and mixed system

As-supplied and processing essentials

Components
Two components
Resin and hardener require controlled mixing before application.
Mix ratio
2:1 by volume
Alternative weight ratio: 100:55, resin to hardener.
Working life
20 minutes
Typical value at 23°C; larger quantities or higher temperatures reduce the available work time.
Tack-free time
40 minutes
Typical surface condition after mixing and room-temperature application.
Technical data

Typical properties before cure

Typical reference values for the resin, hardener, and mixed adhesive. Values are not product specifications.

Property Value Unit Method or condition
Resin appearance Pale yellow liquid — As supplied
Resin specific gravity 1.0 — At 23°C
Resin viscosity 65,000 mPa·s (cP) Brookfield RVT at 25°C; spindle 7, 20 rpm
Hardener appearance Yellow liquid — As supplied
Hardener specific gravity 1.1 — At 23°C
Hardener viscosity 7,000 mPa·s (cP) Brookfield RVT at 25°C; spindle 6, 50 rpm
Mixed appearance Off-white — After resin and hardener are combined
Mixed specific gravity 1.03 — At 23°C
Mixed viscosity 65,000 mPa·s (cP) Brookfield RVT at 25°C; spindle 7, 20 rpm
Preparation, dispensing and cure

Processing LOCTITE® EA E-20HP

Remove paint, oxide films, oils, dust, mold-release agents, and other contaminants from the bonding surfaces. Apply the mixed adhesive evenly to the surfaces, assemble promptly, and keep parts from moving while the bond develops. Higher temperatures accelerate cure, while larger mixed quantities and higher temperatures reduce working life.

Mix ratio: 2:1 resin to hardener by volume, or 100:55 by weight.
Cartridge start-up: Confirm that both components extrude, attach a new static mixing nozzle, and discard approximately 25 to 50 mm of mixed material before bonding.
Application window: Typical working life is 20 minutes at 23°C; apply and assemble promptly.
Cure development: Typical tack-free time is 40 minutes. Representative cured-property data are based on 5 days at 23°C unless otherwise stated.
Storage and handling

Store unopened containers in a dry location at an optimal temperature of 8°C to 21°C. Storage below 8°C or above 28°C can adversely affect product properties. Keep containers closed, protect them from contamination, and do not return material removed during use to the original container. Use appropriate gloves, eye protection, and ventilation for the task.

Cured adhesive

Typical cured properties

Glass transition temperature
60°C
TMA, ISO 11359-2; cured 5 days at 23°C.
Shore hardness
80 Shore D
ISO 868; cured 5 days at 23°C.
Elongation at break
8%
ISO 527-3; cured 5 days at 23°C.
Tensile strength
39 N/mm²
5,700 psi; ISO 527-2; cured 5 days at 23°C.
Dielectric breakdown strength
20 kV/mm
IEC 60243-1; cured 5 days at 23°C.
Substrate-specific performance

Typical bond-strength data

The adhesive was cured for 5 days at 23°C. Results are specific to the listed substrate, preparation, cure, and test configuration and are not universal design values.

Property Value Unit Method or condition
Lap shear - mild steel, grit blasted 22.6 N/mm² (3,270 psi) ISO 4587
Lap shear - aluminum, acid etched and abraded 28.2 N/mm² (4,090 psi) ISO 4587
Lap shear - aluminum, anodized 17.4 N/mm² (2,530 psi) ISO 4587
Lap shear - stainless steel 22.0 N/mm² (3,190 psi) ISO 4587
Lap shear - polycarbonate 3.9 N/mm² (560 psi) ISO 4587
Lap shear - nylon 1.8 N/mm² (260 psi) ISO 4587
Lap shear - fir wood 11.4 N/mm² (1,660 psi) ISO 4587
Block shear - PVC 7.9 N/mm² (1,140 psi) ISO 13445
Block shear - ABS 10.4 N/mm² (1,510 psi) ISO 13445
Block shear - epoxyglass 28.6 N/mm² (4,140 psi) ISO 13445
Block shear - acrylic 2.0 N/mm² (290 psi) ISO 13445
Block shear - glass 32.3 N/mm² (4,690 psi) ISO 13445

Performance evidence

Typical laboratory data show how the cured adhesive responds to selected environmental exposures, elevated-temperature testing, and dry-concrete bonding. These results apply to the stated specimens and conditions.

Chemical and solvent resistance

Retained lap-shear strength is shown as a percentage of initial strength after exposure.

Environment Exposure temperature (°C) 500 h (% initial strength) 1000 h (% initial strength)
Air 87 — 137
Motor oil (10W30) 87 164 171
Unleaded gasoline 87 108 82
Water/glycol 50/50 87 121 125
Salt fog 23 — 73
95% RH 38 — 100
Condensing humidity 49 — 90
Water 23 — 81
Acetone 23 76 95
Isopropanol 23 87 125
Cured 5 days at 23°C on steel with no induced gap; aged at the listed temperature and tested at 23°C by ISO 4587 lap shear.
Temperature and dry-concrete performance
  • In hot-strength testing on acid-etched and abraded aluminum, retained lap-shear strength decreased as test temperature increased. Test specimens were cured 12 hours at 65°C plus 4 hours at 23°C with a 0.1 to 0.2 mm bondline.
  • In a modified ASTM C881/C882-99 test on dry concrete, the concrete fractured before the adhesive failed. The adhesive is not recommended for use on wet surfaces.
Typical results are configuration-specific; verify performance with the intended substrates, preparation, bondline, cure, and service environment.
General industrial bonding

Applications

LOCTITE® EA E-20HP is intended for general industrial assemblies that require a moderate working life and room-temperature cure. Confirm performance on the exact substrate grade, surface condition, joint geometry, and service environment.

Prepared metal components positioned for epoxy adhesive bonding
Metal assemblies
For evaluation in industrial joints using prepared mild steel, aluminum, and stainless steel. Surface contaminants and oxide films should be removed before bonding.
Plastic and composite parts prepared for epoxy adhesive assembly
Plastics and composites
Typical shear data are available for polycarbonate, nylon, PVC, ABS, acrylic, and epoxyglass. Suitability should be confirmed for the exact polymer grade and surface condition.
Dry concrete, wood, glass, and architectural materials for adhesive bonding
Dry concrete and architectural materials
For evaluation on dry concrete, fir wood, glass, and other architectural materials. The adhesive is not recommended for wet-surface bonding.
Next steps

Evaluate LOCTITE® EA E-20HP for your assembly

Krayden can help review substrate combinations, surface preparation, dispense format, working time, bondline control, cure conditions, and environmental requirements for your industrial bonding process.

Leading Brands Trust in Our Products and Services