LOCTITE EA 9394C-2

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LOCTITE EA 9394C-2

Main features

  • 1-Hour 204 deg C Cure
  • Extended Working Window for Controlled Assembly Operations
  • Qualified to MMM-A-132 Type Ii

Product Description

LOCTITE EA 9394C-2 AERO is a two-component, elevated-temperature-cure structural epoxy paste adhesive for aerospace bonding. The system combines a gray Part A with a purple-dark green Part B at a 100:20 mix ratio by weight. A 7-hour pot life at 25°C for a 450 g mass provides an extended working window for controlled assembly, while a 1-hour cure above 93°C develops normal performance. On phosphoric-acid-anodized 2024-T3 aluminum, typical tensile lap shear is 34.5 MPa at 25°C and 11.7 MPa at 204°C. The adhesive is qualified to MMM-A-132 Type II and has an approximate service-temperature criterion of 232°C based on retaining 6.9 MPa lap shear per ASTM D1002.

Key features

  • Extended pot life: 7 hours at 25°C for a 450 g mixed mass, tested by ASTM D2471.
  • Controlled two-part mixing: 100:20 Part A-to-Part B ratio by weight.
  • Elevated-temperature cure: 1 hour above 93°C to achieve normal performance.
  • High-temperature lap shear: typical 11.7 MPa at 204°C on prepared 2024-T3 aluminum after the stated cure.
  • Thermal-aging evidence: typical 16.2 MPa lap shear after 12,000 hours at 177°C, tested at 177°C.
  • Qualification: MMM-A-132 Type II.

Technical Specifications

No specifications available.

Additional Information

Structural epoxy adhesive

LOCTITE EA 9394C-2 AERO

LOCTITE EA 9394C-2 AERO is a two-part structural epoxy paste designed for elevated-temperature cure and high-temperature service in aerospace bonding. It combines an extended pot life with a non-aromatic amine curing agent and retains measurable lap shear strength at temperatures above 204°C under the stated prepared-aluminum test configuration.

Two-part structural epoxy paste Elevated-temperature cure Non-aromatic amine curing agent

LOCTITE EA 9394C-2 AERO two-component adhesive system.

Uncured and component properties

Mix ratio
100:20 by weight
Use the specified Part A-to-Part B weight ratio. Volume measurement is not recommended for structural applications.
Pot life
7 hours at 25°C
Typical value for a 450 g mixed mass measured by ASTM D2471 in a water bath.
Property Value Unit Method / condition
Part A color Gray — As supplied
Part B color Purple-dark green — As supplied
Part A viscosity 650 Pa·s 25°C; Brookfield HBT, spindle 7 at 2.09 rad/s
Part B viscosity 0.04 Pa·s 25°C; Brookfield LVF, spindle 1 at 3.17 rad/s
Part A density 1.45 g/mL As supplied
Part B density 1.00 g/mL As supplied
Processing

Mixing, application, and cure

Accurate weighing, complete mixing, controlled batch size, prepared bonding surfaces, and elevated-temperature cure are required to develop the stated performance.

Component conditioning: Bring the separate components close to room temperature, approximately 25°C, before mixing.
Mixing: Combine Part A and Part B at 100:20 by weight and mix thoroughly. Do not use volume measurement for structural applications unless special ratio-control precautions are in place.
Batch-size control: Do not mix quantities greater than 450 g. Excessive heat buildup can cause uncontrolled decomposition and toxic fumes.
Application and assembly: Apply to clean, dry, properly prepared bonding surfaces and hold the parts in contact until the adhesive is set.
Cure: Cure for 1 hour above 93°C to achieve normal performance.
Cleanup: Remove uncured excess from the work area and equipment before the adhesive hardens, using a suitable cleaning method and applicable solvent-safety controls.
Storage and handling

Store Part A at or below -18°C; refrigerated storage is recommended to maintain product quality. Store Part B at or below 25°C in a cool, well-ventilated area with the container tightly closed. Follow current container labels for shelf-life and component-specific handling requirements.

Cured properties

Approximate service-temperature criterion
232°C
Defined as the temperature at which the adhesive retains 6.9 MPa lap shear by ASTM D1002.
Shore D hardness
84
Tested at 25°C on an approximately 6.35 mm thick specimen after a 1-hour cure at 93°C.
Typical lap shear at 25°C
34.5 MPa
ASTM D1002 on phosphoric-acid-anodized 2024-T3 aluminum after a 1-hour cure at 93°C.
Property Value Unit Method / condition
Ultimate compressive strength at 25°C 32,000 / 220.7 psi / MPa ASTM D695; cylindrical specimen 35.6 mm tall × 14 mm diameter; cured 1 hour at 93°C
Ultimate compressive strength at 121°C 17,000 / 117.2 psi / MPa ASTM D695; cylindrical specimen 35.6 mm tall × 14 mm diameter; cured 1 hour at 93°C

Performance evidence

The following typical results preserve the tested substrate, surface preparation, cure, temperature, and exposure conditions needed to evaluate the adhesive.

Tensile lap shear across test temperature
Test temperature (°C) Typical strength (psi) Typical strength (MPa)
-55 3,500 24.1
25 5,000 34.5
82 4,000 27.6
121 3,200 22.0
149 3,000 20.7
177 2,500 17.2
204 1,700 11.7
232 1,200 8.3
260 800 5.5
ASTM D1002; 2024-T3 bare aluminum adherends phosphoric-acid anodized per ASTM D3933; cured 1 hour at 93°C.
Thermal-aging performance at 177°C
Thermal-aging exposure Typical strength (psi) Typical strength (MPa)
No exposure 2,443 16.8
1,000 hours 2,784 19.2
2,000 hours 2,589 17.9
5,000 hours 2,613 18.0
12,000 hours 2,355 16.2
Tensile lap shear tested at 177°C after the stated exposure duration.
MMM-A-132 Type II conditioning performance
Conditioning Typical strength (psi) Typical strength (MPa)
48 hours at 25°C 5,490 37.9
10-minute soak at 149°C 3,100 21.4
192 hours at 149°C 3,230 22.3
10-minute soak at -55°C 3,880 26.8
MIL-H-83282 hydraulic oil, 7 days at 25°C 5,640 38.9
JP-4 jet fuel, 7 days at 25°C 5,640 38.9
30 days at 49°C and 95–100% RH 5,260 36.3

Additional results: fatigue strength of 750 psi (52 bar) for 106 cycles at 25°C; creep rupture under 1,600 psi (110 bar) for 192 hours was less than 0.1 mil at both 25°C and 149°C.

Conditioned tensile lap shear results were tested at 25°C. Values apply to the stated test configuration and are not universal design allowables.
Next steps

Evaluate LOCTITE EA 9394C-2 AERO for your bonding process

Contact Krayden to discuss substrate preparation, mix and batch controls, cure requirements, temperature-dependent strength data, or qualification considerations for your structural bonding application.