LOCTITE 9430

Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other

LOCTITE 9430

Main features

  • 4,700 psi Lap Shear
  • 50-Minute Working Window
  • Up to 0.1-Inch Gap Bonding

Product Description

LOCTITE® EA 9430 is a two-part, modified epoxy structural adhesive that cures at room temperature. It combines high peel and shear strength with a tough, flexible cured profile for bonding a variety of substrates, including dissimilar materials. The off-white mixed adhesive has a typical 50-minute pot life at 77°F for a 250-gram batch and accommodates bondlines up to 0.1 inch. Cured bonds resist water, salt spray, and many common industrial fluids. Ultimate properties develop in five days at room temperature, while elevated-temperature curing up to 180°F can shorten the cure time.

Key features

  • High peel and shear strength: Typical values include 4,700 psi lap shear and 60 pli peel strength under the specified test conditions.
  • Long working time: Provides a typical 50-minute pot life at 77°F for a 250-gram mixed quantity.
  • Tough, flexible bonding: Supports dissimilar-substrate assemblies and bondline thicknesses up to 0.1 inch.

Applications / Suitable for

  • Bonding dissimilar substrates
  • Assemblies requiring bondlines up to 0.1 inch
  • Bonded structures exposed to water, salt spray, or common industrial fluids
Product Family

LOCTITE 9430

Loading pricing…

TDS, SDS & Technical Documents

Technical Specifications

No specifications available.

Additional Information

Technical properties

As-supplied / before-processing properties

Typical properties of the separate components and mixed adhesive. Values are not guaranteed specifications.

Property Value Unit Method / condition
Pot life 50 min Mixed adhesive at 77°F; 250-gram quantity
Mixed color Off-white — Part A is cream; Part B is clear
Viscosity 200,000–400,000 cP Part A
Viscosity 40 cP Part B
Viscosity 12,000 cP Mixed adhesive
Specific gravity 1.12 — Mixed adhesive
Mix ratio by weight 100:23 Part A:Part B Bulk mixing ratio
Mix ratio by volume 3.78:1 Part A:Part B Bulk mixing ratio
Technical properties

After-processing / final-state properties

Typical cured-material and bonded-joint properties. Strength values apply only to the stated substrates, preparation, cure schedules, and test conditions.

Property Value Unit Method / condition
Tensile strength 5,300 psi ASTM D638
Tensile modulus 380,000 psi ASTM D638
Elongation 6.0 % ASTM D638
Hardness 75 Shore D Typical cured-material value
Lap shear strength 5,000 psi ASTM D1002; etched aluminum; cured 5 days at 77°F; tested at −67°F
Lap shear strength 4,700 psi ASTM D1002; etched aluminum; cured 5 days at 77°F; tested at 77°F
Peel strength 60 pli ASTM D3167; etched aluminum; cured 3 days at 77°F