DEVCON FLEXANE 94

Harmonization Code : 3907.30.00.40 | Epoxy Mold Compounds containing by weight more than 70 % silicon dioxide

DEVCON FLEXANE 94 DEVCON FLEXANE 94

Main features

  • 6,000 cP Castable Urethane
  • Replacement-Part and Flexible-Mold Fabrication
  • 19.3 MPa Cured Tensile Strength

Product Description

Devcon® Flexane® 94 Liquid is a low-viscosity, castable, non-shrinking urethane compound that cures at room temperature to a rigid rubber material. The black, two-component system has a mixed viscosity of 6,000 cP, a 10-minute pot life at 24°C, and a 5-hour demolding time. It is designed to reproduce low- to medium-volume or discontinued rubber parts, form flexible molds and non-scratching fixtures or linings, and encapsulate wire and electronics exposed to impact, vibration, expansion, and contraction. Typical cured properties include 97 Shore A hardness, 500% elongation, 19.3 MPa tensile strength, and 14 kV/mm dielectric strength.

Key features

  • Castable low-viscosity urethane: Mixed viscosity of 6,000 cP supports controlled pouring and mold filling.
  • Room-temperature cure: No applied heat is required for the documented cure process.
  • Five-hour demolding: Supports removal from the mold after the documented demolding interval.
  • Rigid rubber final state: Cures to a black material with typical hardness of 97 Shore A.
  • High elongation and tear resistance: Typical cured values include 500% elongation and 73 N/mm tear resistance.
  • Molding, fixturing, lining, and encapsulation: Supports flexible molds, replacement rubber parts, non-scratching fixtures or linings, and wire or electronics encapsulation.

Applications / Suitable for

  • Reproduction of low- to medium-volume or discontinued rubber parts
  • Flexible molds and forming dies
  • Non-scratching holding fixtures and protective linings
  • Encapsulation of wire and electronics exposed to impact, vibration, expansion, or contraction
Product Family

DEVCON FLEXANE 94

Loading pricing…

TDS, SDS & Technical Documents

Technical Specifications

No specifications available.

Additional Information

Adhesives | Castable Urethane Compound

Devcon® Flexane® 94 Liquid

Devcon Flexane 94 Liquid is a castable, non-shrinking urethane that cures at room temperature to a rigid rubber material. Its low mixed viscosity supports pouring into molds, fixtures, linings, and encapsulation cavities, while the cured material combines 97 Shore A hardness with high elongation and tear resistance.

6,000 cP mixed viscosity 10 min pot life 5 hr demolding 97 Shore A 500% elongation

 

Product data

As-Supplied Properties

Typical uncured and mixed product data at 72-75°F (23-24°C), unless otherwise stated. Values are representative and are not specifications.

Property Value Unit Method / condition
Color Black — Mixed material
Mix ratio by weight 69 : 31 — Resin : curing agent
Mixed viscosity 6,000 cP 72°F (23°C)
Pot life 10 min 75°F (24°C)
Specific volume 26.5 (0.957) in³/lb (cm³/g) Mixed material
Coverage at 1/4 in (6.35 mm) 106 (1,508) in²/lb (cm²/kg) Theoretical coverage
Application

Surface Preparation, Mixing, and Application

Prepare and prime the substrate for the required adhesion level, condition the Flexane components to 65-85°F (18-29°C), mix until the material is uniform and streak-free, then pour from one side of the mold or cavity to help displace air.

Conditioning and mix ratio: Condition to 65-85°F (18-29°C) and combine 69 parts resin with 31 parts curing agent by weight.
Pot life and demolding: Pot life is 10 minutes at 75°F (24°C); documented demolding time is five hours.
Cure progression: Allow 10 hours before light service, 16 hours for functional cure, and seven days at 70°F (21°C) for full cure.

 

Application Sequence

Stage 1
Clean, roughen, and prime
Remove oil, grease, and dirt. Roughen metal or rubber as directed. For maximum adhesion on metal, sandblast to a 2-3 mil profile and near-white SSPC-SP5 finish, then prime immediately to limit oxidation.
Stage 2
Mix to a uniform consistency
For 1 lb units, mix for two minutes while scraping the sides and bottom, transfer to the supplied plastic container, and mix for two additional minutes. For 10 lb units, use a suitable propeller mixer for approximately 4-6 minutes and keep the propeller submerged to limit entrained air.
Stage 3
Brush, pour, de-air, and cure
Brush a thin coat over the substrate, then pour from one side. Gently pass hot air over the surface to break visible bubbles without overheating. Allow the documented demolding, light-service, functional-cure, and full-cure intervals before loading.

Primer and Surface Guidance

Substrate Primer Preparation guidance
Metal FL-10 Primer Clean and roughen. For maximum tear resistance, moisture exposure, or water immersion, use FL-10 and FL-20.
Rubber FL-20 Primer Clean and roughen until the surface appears new or deeper in color. Use FL-10 on hard-to-bond rubber; porous rubber may require multiple coats.
Wood FL-20 Primer Confirm the substrate is clean, dry, and structurally sound before priming.
Fiberglass FL-20 Primer Remove contamination and prepare the surface before applying the primer.
Concrete FL-20 Primer Use on clean, dry, sound concrete and validate adhesion under the intended conditions.
Rigid plastics FL-20 Primer - two coats Confirm plastic compatibility and validate the complete preparation and cure process.
Storage and Handling

Store Devcon Flexane 94 Liquid in a cool, dry place. The technical data sheet lists 1 lb kit and 10 lb order configurations, while the current manufacturer product page also identifies NSN 8030-01-036-9228. Use only for industrial applications and consult the current SDS for complete handling, exposure-control, first-aid, storage, and disposal requirements.

Final rubber state

Cured Properties

Typical cured data after seven days at 75°F (24°C), unless otherwise stated. Values are representative and should not be used as design allowables.

Property Value Unit Method / condition
Hardness 97 Shore A ASTM D2240
Tensile strength 2,800 (19.3) psi (MPa) ASTM D412
Maximum elongation 500 % ASTM D412
Tear resistance 415 (73) pli (N/mm) ASTM D624
Dielectric strength 350 (14) V/mil (kV/mm) ASTM D149
Cured shrinkage 0.0014 in/in (cm/cm) ASTM D2566
Maximum operating temperature - dry 180 (82) °F (°C) Documented limit
Maximum operating temperature - wet 120 (49) °F (°C) Documented limit
Solids by volume 100 % Cured material

Chemical Resistance

Chemical Rating Test context
1,1,1-Trichloroethane Poor Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Aluminum sulfate, 10% Very good Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Cutting oil Fair Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Gasoline, unleaded Poor Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Hydrochloric acid, 10% Very good Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Hydrochloric acid, 36% Very good Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Isopropanol Poor Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Methyl ethyl ketone Poor Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Phosphoric acid, 10% Very good Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Potassium hydroxide, 40% Very good Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Sodium hydroxide, 50% Very good Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Sodium hypochlorite Very good Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Xylene Poor Seven-day room-temperature cure; 30-day immersion at 75°F (24°C)
Supported use contexts

Applications

Devcon Flexane 94 Liquid supports castable urethane applications where the selected substrate, primer, mold design, processing method, cure schedule, hardness, and service environment are suitable for the finished part or encapsulated assembly.

Replacement rubber parts
Reproduce low- to medium-volume or discontinued rubber parts using a prepared mold and a validated pouring and cure process.
Molds, fixtures, and linings
Form flexible molds, forming dies, non-scratching holding fixtures, and protective linings that use the documented rigid-rubber hardness and castable processing.
Wire and electronics encapsulation
Encapsulate wire and electronics exposed to impact, vibration, expansion, and contraction when the cured properties and service-temperature limits are suitable.
Next steps

Technical Support

Work with Krayden to evaluate Devcon Flexane 94 Liquid against your mold or part geometry, substrate, primer selection, mixing equipment, pour depth, air-release method, cure schedule, hardness, chemical exposure, and service temperature. Our team can help review packaging, process trials, compatibility, and implementation requirements.

Leading Brands Trust in Our Products and Services

Products that Perform| Knowledge that Serves| Service that Delivers